ʻO Titanium gypsum kahi ʻano ʻōpala me ka dihydrate gypsum ma ke ʻano nui, i hana ʻia ma ka hoʻohui ʻana i ka lime (a i ʻole calcium carbonate) e hoʻokaʻawale i ka nui o ka wai ʻawaʻawa i mea e mālama ai i ka wai ʻawaʻawa i ka wā e hana ʻia ai ka titanium dioxide e ka sulfuric acid method. ʻO ka hoʻokuʻu ʻana o ka titanium gypsum ʻaʻole wale ka nui o ka ʻāina a hoʻohaumia i ke kaiapuni, akā ke kumu hoʻi i ka ukana waiwai nui i nā ʻoihana titanium dioxide. Hiki ke hoʻohana ʻia ka Titanium gypsum e hana i ka mea hoʻopaʻa sima ma hope o ka hana ʻia ʻana e ka mīkini wili. ʻO Guilin Hongcheng kahi mea hana ʻoihanatitaniumwili palaoa gypsum.ʻO kēia ka wehewehe ʻana pehea e hoʻomākaukau ai i ka titanium gypsum composite cementitious material me ka hana maikaʻi.
titaniumwili palaoa gypsum-HC pendulum Raymond mill
1. He aha ka hopena o ka hoʻohui ʻana i nā admixtures like ʻole i ka titanium gypsum i kāna hana?
ʻO ka waiwai ikaika o ka titanium gypsum ma hope o ka hoʻololi kino ʻana he ʻokoʻa me ka gypsum kūlohelohe a me nā gypsum kemika ʻē aʻe. Pono e hoʻohui ʻia kekahi mau mea hoʻohui e hoʻomaikaʻi i ka waiwai o ka titanium gypsum. ʻO nā mea hoʻohui i hoʻohana ʻia me ka lehu desulfurization, ka lehu lele, ka wai kinai ʻia, ka alum, ka mea hoʻemi wai a me ka retarder.
Ke hoʻohana ʻia ka slag i hoʻopau ʻia i ka wai e like me ka aggregate māmā, ke emi ka ʻike ma mua o 40%, ʻaʻole ia e hoʻopilikia i ka ikaika o ka huahana gypsum titanium, a hiki ke hoʻemi pono i ka nui o ka nui o ka huahana; Ke emi ka maʻiʻo o ka lehu lele ma mua o 30%, he hopena liʻiliʻi ia i ka hoʻomaikaʻi ʻana i ka ikaika o ka titanium gypsum, akā inā ʻoi aku ka nui o ka lehu lele ma mua o 30%, e hōʻemi ia i ka ikaika o ka titanium gypsum, a kōkua ka lehu lele e hoʻomaikaʻi i ka ikaika hope o ka titanium gypsum (7d). Hiki i ka lehu desulfurized ke hoʻomaikaʻi nui i ka ikaika o ka titanium gypsum. Me ka hoʻonui o kāna ʻike, hiki ke hoʻomaikaʻi nui ʻia ka ikaika o nā huahana gypsum titanium. Hiki i ka Alum ke hoʻomaikaʻi maikaʻi i ka ikaika o ka titanium gypsum, a inā he 3% ka ʻike, ʻoi aku ka maikaʻi o ka hopena; ʻO ka nui o ka wai i hoʻohui ʻia he hopena maopopo i ka ikaika o ka titanium gypsum. Me ka hoʻonui ʻana i ka nui o ka wai i hoʻohui ʻia, emi nui ka ikaika o ka hāpana. No laila, ʻoiai e hōʻoiaʻiʻo ana i ka wai o ka gypsum paste, ʻoi aku ka haʻahaʻa o ka nui o ka wai i hoʻohui ʻia, ʻoi aku ka maikaʻi.
Ma ke ʻano he māmā, hiki ke hoʻomaikaʻi i ka wai hoʻopau i ka nui o nā huahana hoʻāʻo titanium gypsum. ʻO ka lehu desulfurized, ka lehu lele a me ka alum hiki ke hoʻomaikaʻi nui i ka hana ikaika o ka titanium gypsum. No laila, koho ʻia ka titanium gypsum, ka lehu desulfurized a me ka lehu lele e like me ka pauka, hoʻohana ʻia ka slag i hoʻopau ʻia i ka wai e like me ka aggregate māmā, a hoʻohana ʻia ka alum, melamine a me ka waikawa citric e like me nā mea hoʻohui. Loaʻa nā ʻāpana maikaʻi loa ma ka hoʻololi ʻana i ka māhele o ka pauka. ʻO ka hapa o ka aggregate he 40% o ka pauka, ʻo ka hapa o ka alum i ka additive he 3% o ka pauka, ʻo ka hapa o ka melamine a me ka citric acid he 1% kēlā me kēia, a me ka hoʻohui ʻana o ka titanium gypsum 70% a me ka lehu desulfurized 30%, maikaʻi ka hana o ka mea cementitious.
2. Pehea e hoʻomākaukau ai i ka titanium gypsum composite cementitious mea me ka hana maikaʻi?
Ma hope o ka calcining no 2h ma 600 ℃, hoʻohui ʻia ka titanium gypsum me ka lehu lele, slag a me ka sima e hoʻopōkole i ka manawa hoʻonohonoho mua o ka composite i 3h, ka manawa hoʻonohonoho hope i 5h, a ʻo ka ikaika flexural 28d a me ka ikaika compressive hiki i 4.3MPa a me 13.6MPa pākahi. Me ka titanium gypsum a me ka slag ma ke ʻano he kumu kumu, hiki ke hoʻohana ʻia ka clinker sima a me ka mea hoʻohaʻahaʻa wai ikaika mua e hoʻomākaukau ai i ka sima me ka hana maikaʻi loa, a ʻoi aku ka maikaʻi o kona ikaika a me ke kūpaʻa wai ma mua o ke kūkulu ʻana i ka gypsum. Hōʻike ka noiʻi ʻana i ka ikaika o ka titanium gypsum i hui pū ʻia i nā mea cementitious ma hope o ka hoʻōla maoli ʻana no nā lā 28 hiki ke hoʻokō i nā koi o ke kūkulu ʻana i nā mea pā hale a me nā mea i hui pū ʻia me ke ala o ke alanui, ʻoi aku ka liʻiliʻi o kona dissolution ma mua o 20% o ka hale gypsum, a ʻo ka nui o ka absorption wai ma kahi o 50% o ke kūkulu hale gypsum, e hōʻike ana i ka maikaʻi o ka titanium composite gypsum. Inā ʻaʻole i hui pū ʻia ka titanium gypsum fly ash slag composite cementitious material me activator, lōʻihi kona manawa hoʻonohonoho a haʻahaʻa kona ikaika mua. ʻO ka hoʻohui ʻana i ka nui kūpono o ka sima i kēia mea hoʻohuihui ʻia e hiki ke hoʻopōkole i ka manawa hoʻonohonoho o ka mea hoʻohuihui ʻia, kahi kūpono i ka ulu ʻana o ka ikaika o ka mea hoʻohuihui.
Kekahi mau noiʻi hopena hōʻike i ka hoʻohui ʻana i ka 5% sima i ka titanium gypsum lele lehu slag composite cementitious mea hiki ke hoʻopōkole i ka manawa hoʻonohonoho mua o ka mea i hoʻohui ʻia i 4h, ka manawa hoʻonohonoho hope i 9h, a me ka 28d flexural ikaika a me ka ikaika compressive hiki ke hiki i 5.8MPa a me 29.OMPa pakahi. Hiki ke hoʻomākaukau ʻia nā mea hana kiʻekiʻe composite cementitious ma o ka hoʻohana ʻana i ka titanium gypsum, lele lehu, slag a me kahi liʻiliʻi o Portland cement a clinker paha, ke koho ʻana i ka mea hoʻoulu kūpono a lawe i nā kaʻina hana kūpono. Hōʻike ka noiʻi ʻana i ka hoʻohui ʻana i ka 5% alunite i loko o ka titanium gypsum fly ash slag composite cementitious mea hiki ke hoʻopōkole i ka manawa hoʻonohonoho mua o ka mea hoʻohuihui cementitious i 1h, ka manawa hoʻonohonoho hope i 2h, a me ka ikaika flexural 28d a me ka ikaika compressive hiki i 9.5 MPa a me 53.0 MPa i ka ikaika maʻamau o Portland 53.0.
3. Pehea e pili ai nā ʻano mea hana like ʻole i ka ikaika o ka titanium gypsum composite cementitious?
Hiki ke hoʻomaikaʻi nui ʻia ka ikaika o nā mea cementitious composite ma hope o ka calcination o ka titanium gypsum. Ua hoʻonui ʻia ka ikaika 28d o ka mea hoʻoheheʻe ʻia e ka sima wale nō i ka 70%, a ua hoʻonui ʻia ka ikaika flexural a me ka compressive o ka mea hoʻohui me ka piʻi ʻana o ka ʻike cement. Ke 15% ka nui o ka sima, ʻo kona ikaika ka mea kiʻekiʻe loa. I ka 15% o ka lime, 0 ka nui o ka sima, a ʻo kona ikaika ka haʻahaʻa loa. I ka calcined titanium gypsum fly ash system, ʻoi aku ka maikaʻi o ka hoʻohana ʻana i ka cement excitation i ka hoʻomaikaʻi ʻana i ka ikaika o ka ʻōnaehana.
Inā pono ʻoetitaniumwili palaoa gypsum, please contact mkt@hcmilling.com or call at +86-773-3568321, HCM will tailor for you the most suitable grinding mill program based on your needs, more details please check www.hcmilling.com.E hoʻolālā kā mākou ʻenekini koho i ka hoʻonohonoho ʻana i nā mea hana ʻepekema no ʻoe a me ka ʻōlelo no ʻoe.